General Leather Retanning Process

2008/8/9 10:19:00 41741

The amount of material used is calculated as blue leather weight.

Wash: 300% water (20 degrees), turn LOMIN, row bath.

Wash: 300% water (20 degrees), turn 5 min, row bath.

Neutralization: 200% water (20 centigrade), 1.5% baking soda, turn 50min, row bath.

Wash: 300% water (50 degrees), turn LOMIN, row bath.

Dyeing: 200% water (50 degrees), 0.5% dye, 30min, x% formic acid (pH=3.5 3.6), turn LOMIN, row bath.

Fatliquoring: 100% water (50 centigrade), 1.5% sulfated fish oil, 1.5% calf oil, 30min, x% formic acid (pH3.5 3.6), turn l0min.


  • Related reading

Structure And Design Of Sports Shoes

Shoemaking technology
|
2008/8/9 10:18:00
41752

Method For Manual Cutting Of Leather

Shoemaking technology
|
2008/8/9 10:17:00
41752

Seven Themes Of Fashion Trends In 2009

Shoemaking technology
|
2008/8/9 10:16:00
41899

Production Process Of Polyurethane Material For Sole

Shoemaking technology
|
2008/8/9 10:13:00
41744

Surface Treatment Of Leather Shoes

Shoemaking technology
|
2008/8/9 10:13:00
41765
Read the next article

Influence Factors Of Surface Treatment On Bonding Strength

The surface treatment of adhesive material is one of the most important processes in the whole bonding process. It is also one of the keys to the success and failure of gluing. Because bonding is mainly based on the adhesion of adhesive to the adhesive surface, the surface treatment of adhesive material may become the main factor determining the strength and durability of adhesive joints. However, due to a series of processes such as oxide, rust, oil, adsorbents and adsorbents on the surface of